Disc Spring Stress Relaxation and Residual Load: From a NASA Case Study to Engineering Acceptance Criteria

  • 分类:Share
  • 发布时间:2026-11-24 09:39:35

【概要描述】Learn how high temperatures affect disc spring load retention and preload. Explore NASA test findings, material selection, stress relaxation and engineering acceptance criteria.

Disc Spring Stress Relaxation and Residual Load: From a NASA Case Study to Engineering Acceptance Criteria

【概要描述】Learn how high temperatures affect disc spring load retention and preload. Explore NASA test findings, material selection, stress relaxation and engineering acceptance criteria.

  • 分类:Share
  • 发布时间:2026-11-24 09:39:35
  • 访问量:
详情

During valve maintenance, the nuts may still be in place while the compressive force on the packing has already decreased. The key question for designers is how much force the disc springs can still apply to the seal before the next maintenance interval. To answer this, the disc spring body temperature, installed height and holding time must first be specified; the load is then measured at the end of the test. Through long-term work with customers in valves, petrochemicals and high-temperature equipment, Raleigh Spring has found that many disputes over sealing failures originate in designs that consider only room-temperature load curves and overlook preload loss caused by long-term relaxation at elevated temperatures.

Why does the load decrease at the same compressed height?

A disc spring generates axial force through elastic deformation of its conical section. When it is compressed between two parallel platens, the distance between the platens is fixed. At elevated temperatures, the material may gradually undergo permanent deformation, reducing the elastic deformation that carries the load. As a result, even if the platens do not move, the load-cell reading can decrease. This is load relaxation under constant-height conditions.

d9ff93f1-6d39-47b6-a738-7a2045fe69e8.png

Figure 1. Axial cross-section schematic of a disc spring. The two green sections represent the same disc spring. H is the platen spacing at the test temperature. Arrows indicate axial force; their lengths are illustrative only.

If a constant weight is used instead, the applied force is determined by that weight. The parameter to observe is then how much the disc spring height decreases over time. This is creep. The two tests record different quantities, so the report must state whether height or force is controlled. Raleigh Spring’s disc spring testing laboratory can conduct constant-height stress-relaxation tests and constant-load creep tests, aligned with the requirements of DIN 16983, DIN 2093 and GB/T 1972-2023, and provide measured data for project acceptance.

Choose the correct reference point when calculating load retention

Stabilize the disc spring and fixture at the target temperature, compress the spring to the agreed installed height, and record the hot load at the start of the test as F₀. Maintain the specified spacing and temperature, then record the remaining hot load Fₜ at the agreed time.

Load retention (%) = Fₜ ÷ F₀ × 100%     |     Load loss (%) = (F₀ − Fₜ) ÷ F₀ × 100%

For example, at the same installed height, the load is 10.0 kN at room temperature, 9.0 kN after temperature stabilization, and 8.55 kN after a further 48-hour hold. Load retention during the hold is 95%; relative to the room-temperature assembly value, 85.5% remains. The force available to the equipment at that point is 8.55 kN. These figures are for illustration.

A disc spring stack after 1,178 hours of operation

In an engineering prototype of a Stirling radioisotope generator, the U.S. National Aeronautics and Space Administration (NASA) used a stack of full-hard 302 stainless steel disc springs to clamp a heat-transfer interface. During teardown, the research team found that after 1,178 hours of operation, the stack’s axial preload had fallen from approximately 1,450 N during operation to approximately 670 N.

706aaad5-ef8e-4d03-ab2a-3fc47848139f.png

Figure 2. Two preload readings from the same device, redrawn based on Section 6.2 of the NASA technical memorandum. Both values are approximate; intermediate load values are not provided in that section.

The operating point can shift even when stiffness remains similar

The teardown also found that the disc spring stack’s stiffness had changed very little, while its stack height had shortened by approximately 0.25–0.38 mm. Stiffness describes how much the force increases when the spring is compressed a little further. Once the stack height becomes shorter, the available compression at the same assembly spacing is reduced, and preload decreases accordingly. Therefore, when investigating preload loss, remeasure both the stack height and the load at the specified height. When delivering complete disc spring solutions, Raleigh Spring also identifies the recommended operating-point stress range to help avoid conditions in which high stress accelerates relaxation.

What does retaining roughly half the preload mean?

The report states that the material supplier specified a maximum service temperature of 260 °C, while thermal analysis for the relevant design estimated that the spring seat could reach 250 °C. The latter is the analyzed temperature of the spring seat; the actual temperature of the prototype disc springs remains uncertain. The research team considered material creep the most likely explanation for the change in stack height and noted that the remaining force at that time was still sufficient for the device’s heat-transfer requirements.

Therefore, the approximately 46% figure describes the proportion of preload remaining after the actual operating history of this particular device. To select disc springs for another flange or valve, the disc spring body temperature must be measured and the minimum preload required to maintain the joint’s function must be defined. In a valve packing assembly, for example, the disc springs may recover as the packing consolidates, changing the joint clamping force as well. To distinguish packing compression from relaxation of the disc springs themselves, record the working height of the complete stack and conduct a separate constant-height test on disc springs from the same batch.

The same alloy grade can also produce different load-retention results

The alloy producer Special Metals compared two helical springs of identical geometry made from INCONEL X-750. Both specimens received the same age-hardening treatment and were held for 500 hours at approximately 427 °C under an initial shear stress of approximately 483 MPa. The wire conditions differed in degree of cold work, and the measured load losses were 3% and 12%, respectively.

c9c36350-bad0-4612-960d-b50748911d57.png

Figure 3. Converted from the load-loss values in the producer’s report. The original test conditions were 800 °F and 70 ksi; both groups were aged at 1,350 °F (approximately 732 °C) for 16 hours. The specimens were helical springs, and the percentages apply only to this specific comparison.

What conditions should be checked beyond the material grade?

First, in what condition was the material formed, and what heat treatment and presetting did it receive? In Figure 3, changing only the wire condition resulted in a 9-percentage-point difference between the two specimen groups. For disc springs formed from strip, the material batch, supply condition, heat treatment and presetting process should be recorded for each specimen. Finished products made using the same process should then be tested to verify the target load. For disc spring materials including INCONEL X-750, Inconel 718, 51CrV4 and 302 stainless steel, Raleigh Spring has established corresponding heat-treatment and presetting process databases to reduce relaxation variation between batches.

Second, how far is the disc spring actually compressed? Even with the same material and heat lot, changes in spring dimensions and installed height alter the operating stress. The German manufacturer Christian Bauer’s disc spring handbook provides separate charts by steel grade and reference relaxation curves based on stress, 20 °C or 100 °C, and holding periods of 48 or 1,000 hours. To evaluate a product at 400 °C, data at the corresponding temperature and operating point should be obtained.

Record operating hours separately from start-stop cycles

For long-term clamping, the main concern is the residual force at the end of the specified period. If the equipment repeatedly heats up, cools down, opens or closes, stroke, temperature cycles and cycle count must also be recorded, and fatigue must be evaluated separately. The fatigue-life diagrams in ISO 19690-2 describe life under cyclic loading. To determine the residual force after hundreds of hours at a constant temperature, load-versus-time records are also required. Predicting years of service from 48-hour data requires tests at multiple temperatures and durations, as well as validation that the extrapolation model applies to the material and process concerned. Raleigh Spring can design accelerated relaxation validation plans based on the customer’s required service life, providing a sound basis for long-duration operating conditions.

How to include residual load in acceptance criteria

Working backward from the minimum force required by the equipment is easier to verify than specifying only “temperature resistance up to 400 °C.” Using the illustrative example above, assume the seal requires at least 8.80 kN. Even though the disc springs retain 95% of their load during the hold, the actual remaining force is 8.55 kN—0.25 kN below the requirement.

Agree on a finished-product test that can be repeated

Test stage

Items to be agreed and recorded by both parties

Specimen and assembly

Record drawing number, batch, heat-treatment condition and number of specimens. For a disc spring stack, assemble it using the actual number of springs, orientation, guidance and contact conditions.

Temperature and height

Measure temperature near the specimen to verify the spring body temperature. Agree on the heating and loading sequence, stabilization criteria and hot spacing. Check fixture thermal expansion and load-measurement zero drift.

Force and time

Record F₀ at the agreed starting point, maintain the hot spacing, and continuously record load or read Fₜ at the agreed time. If a separate measurement is made after cooling, report the cold result separately.

Evaluation and report

Report the initial force, final force, retention ratio and minimum final force for each specimen. Agree on how tolerances and measurement uncertainty will be handled, and validate long-term requirements against the actual service duration.

A technical clause that can be adapted directly

For a 48-hour acceptance test, stabilize the disc spring body at 400 °C, compress it to the hot installed height H specified on the drawing, and start timing. Maintain this temperature and height for 48 hours. The remaining hot axial force of each specimen must be at least 8.80 kN. The report shall list the initial force, final force and measured temperature for each specimen. The specific height, tolerances and sampling quantity shall be agreed by both parties for each project.

References

NASA Glenn Research Center (2018), Investigation of Anomalies on the Second Engineering Unit of the Advanced Stirling Radioisotope Generator, NASA/TM-2018-219400, Section 6.2, p. 18.

Special Metals, INCONEL X-750 Alloy Technical Bulletin, “Springs” section, pp. 16–18; comparison of wire conditions on p. 17.

Christian Bauer, Theory and Practice of Disc Springs, Section 2.8.3, Figures 25 and 26.

International Organization for Standardization, ISO 19690-2:2018, Disc springs—Part 2: Technical specifications, scope and clauses for Grade B disc springs.